Reading Your Dross: Low-Speed, High-Speed, Air and Nitrogen

|Gregg Hinton
Plasma-cut steel edge showing dross along the bottom of the kerf

Dross is the plate talking to you. Every bead hanging off the bottom of a cut is telling you something about your speed, your height, your amperage or your nozzle. The trouble is most operators only hear one word of it: slow down. And about half the time, slowing down is exactly the wrong move.

Here's how to read it.

What dross actually is

Dross is molten metal that didn't get blown out of the kerf. It re-solidifies on the edge of the part instead of leaving with the rest of the spray. Every shop fights it, and every minute spent grinding it off is a minute the cut was supposed to save you.

Three settings decide whether you get dross: cutting speed, amperage and standoff. Same three we covered in Cover Your Amperage, Speed and Standoff. Dross is where you see those three settings show up on the part.

Low-speed dross: thick, bubbly, comes off with a knock

Travel too slow and the arc goes looking for more metal to cut. It widens, the kerf opens up, and the fast-moving core of the jet can't clear the molten metal anymore. It piles up along the bottom edge in a thick, globby bead.

How to recognize it: heavy, rounded, bubbly buildup on the bottom edge. Usually knocks off with a chipping hammer.

What causes it: speed too slow. Too much amperage or too little standoff does the same thing, because all three put more energy into the same spot of plate.

How to fix it:

  • Speed up in small steps. Five inches per minute at a time is a good increment.
  • If speed alone doesn't clear it, raise the standoff a little.
  • Still there? Drop the amperage, or step down to a smaller nozzle for that thickness.

One exception: a bit of low-speed dross in tight corners is normal. The machine has to slow down to make the turn, and the plate notices.

High-speed dross: thin, hard, and welded on

Travel too fast and the arc can't keep up. It lags back in the kerf and leaves a thin, hard bead of uncut metal rolled along the bottom edge. This is the one that costs you real money, because a hammer won't touch it. It's a grinder job.

How to recognize it: a small, tight bead that feels welded to the part. At the extreme, you'll see sparks rooster-tailing off the back of the cut.

What causes it: speed too fast. Standoff too high or amperage too low does the same thing, because both take energy out of the jet.

How to fix it, in this order:

  • Check the nozzle first. A worn orifice — gouged, oversized or out of round — can't focus the arc, and no speed setting will fix that. Our guide to telling when your consumables are worn out shows what to look for.
  • Slow down in small steps.
  • Bring the torch closer to the plate.
  • Add amperage, staying under the nozzle's rating.

Top spatter: the third kind

Sometimes the dross isn't on the bottom at all. Top spatter is a light coating of re-solidified metal sprayed along the top of the part. It comes off easily, but it's an early warning. The usual causes are a worn nozzle, too much speed or too much height. Same first check: look at the nozzle.

Read the lag lines before you touch a setting

The cut face tells you which way to go before the dross does. Look at the lag lines — the small ridges running down the cut surface.

  • Straight up and down: you're slow.
  • A slight lag, about 2–3 degrees: that's the sweet spot.
  • Slanted hard back, curling into an S at the bottom: you're fast.

That slight lag marks the dross-free window: the speed range where the part comes off clean. Your whole job is finding that window and staying in it.

Air vs nitrogen on an air plasma cutter

Air plasma cutters, like the EX-TRAFIRE® and Powermax® lines, are built to run on clean, dry shop air. Most shops never run anything else. But some keep a bottle of nitrogen around, and the question comes up: will it cut cleaner? On mild steel, no.

Watch the arc as it leaves the bottom of the plate. On air, through a proper shade, the arc should come out the bottom with just a slight trail behind the torch. If it's trailing well back, you're going too fast.

Running nitrogen in an air plasma cutter

Expect hard-to-remove dross. That's just the nature of it. Nitrogen has no oxygen in it, so it doesn't run as hot as air does on steel.

Expect to give up capacity. In our experience you lose about 30% of your cut speed and your thickness capacity compared with air.

Where nitrogen earns its place is stainless. On stainless steel it gives you a cleaner, less oxidized cut edge than air does.

In the field, it'll get you through in a pinch. If nitrogen is all you have on site, it will cut. Before you hook it up, check that your machine's manual lists nitrogen as an approved gas, and run it through a regulator set to the machine's inlet pressure.

But for everyday mild steel cutting, we don't recommend it. Stick with clean, dry air.

Air has its own catches

It leaves some nitriding and oxidation on the cut edge. That's not dross, but it can cause porosity if the part gets welded. It's usually handled by running weld wire with deoxidizers and denitriders. Worth knowing before you blame the welder.

It has to be dry. Wet or oily air changes how the arc behaves and chews through consumables. If your dross shows up out of nowhere on a setup that used to cut clean, check your air before you start turning knobs. More on that in Wet Air Is Killing Your Plasma Consumables.

The plate matters too

Not every sheet cuts the same. Cold-rolled steel generally cuts cleaner than hot-rolled, and pickled cleaner than unpickled. If one sheet is fighting you and the last one wasn't, the settings might not be the problem.

The rule that saves the most time

Change one thing at a time. Speed first, in small steps. Then height. Then amperage. If you change two at once and the cut gets better, you don't know which one fixed it, and you'll be lost the next time the thickness changes.

And when a cut does come off clean, write down every setting that made it. That record, from your machine, your air and your plate, is worth more than any chart.

If the nozzle turns out to be the problem, find the right replacement stack for your torch here. Send us the OEM part number if you're not sure, and you'll get a fitment answer quickly.